Click to go to RathGibson home page

347/347H tubing and pipe header image

Physical Properties of 347/347H Alloys in the Annealed Condition at -20°F to +100°F

Tensile Strength Yield Strength
Alloy UNS Designation Spec. psi MPa ksi psi MPa ksi Elongation in 2 inches (min.) % Grain Size Req. Maximum Harndess Modulus of Elasticity(x106 psi) Mean Coefficient of Thermal Expansion IN./IN./°F x 10-6) Thermal Conductivity (BTU-in/ft2-h-°F)
347 S34700 75,000 (515) 30,000 (205) 35 29.0 9.2
347H S34709 75,000 (515) 30,000 (205) 35 7 or coarser 29.0 9.2

Composition of 347/347H tubing and pipe

Grade 347 347H
UNS Designation S34700 S34709
Carbon (C) Max. 0.08 0.04 – 0.10
Manganese (Mn) Max. 2.00 2.00
Phosphorous (P) Max. 0.04 0.04
Sulphur (S) Max. 0.03 0.03
Silicon (Si) Max. 0.75 0.75
Chromium (Cr) 17.0 – 20.0 17.0 – 20.0
Nickel (Ni) 9.0 – 13.0 9.0 – 13.0
Molybdenum (Mo)
Nitrogen (N)
Iron (Fe) Bal. Bal.
Other Elements Cb+Ta=10xC-1.0 Cb+Ta=8xC-1.0

347/347H Product Range

Alloy UNS Designation Werkstoff NR. Specifications*
347 S34700 1.4550 A269, A/SA249, A/SA312
347H S34709 A/SA249, A/SA312

*Note: The specifications noted including ASTM, ASME, or other applicable authorities are correct at the time of publication. Other specifications may apply for use of these materials in different applications.